High-Precision Thermoforming It’s Putting the ‘Pressure’ on Injection Molding

A look at the production of a high-tech medical device shows why pressure forming has injection molders looking over their shoulders. Complex shapes, undercuts, snap-fits, precise styling lines—all of these are within the capabilities of today’s industrial thermoformers.

By Joseph A. Grande, Senior Editor

print this article Print This Article


Learn More
Visit the
Injection Molding Zone

Company Info

Maac Corp.,
Carol Stream, Ill.
800-588-MAAC

Kleerdex Co. LLC,
Aiken, S.C.
(800) 325-3133

Specialty Manufacturing Inc., San Diego
(800) 491-1652

Manufacturers of high-precision, highly styled parts that have historically looked to injection molding have a new option that offers equivalent results with shorter lead times and lower tooling costs. Industrial thermoforming is emerging as a competitor for injection molding, providing the complex geometries and tight tolerances that once were the exclusive domain of injection molders.

Industrial thermoforming
Industrial thermoforming can compete in cost and quality with injection molding for complex, high-precision parts like the enclosure panels for a new medical diagnostic machine.

For high-volume production of small to medium-size parts, injection molding is still more economical and remains the dominant plastics manufacturing process. But for low-volume production of larger parts, industrial thermoforming—particularly pressure forming—has emerged as an attractive alternative. A multi-component enclosure for a medical diagnostic machine is the latest example of how far industrial thermoforming has come in recent years.

Better fit and function
The Skylight Gamma Camera medical-imaging system from Philips Medical Systems, Milpitas, Calif., is the first gantry-free imaging system. The open-floor design permits imaging of a patient in any position, in any bed, and imaging two patients simultaneously. Its thermoformed enclosure panels comprise 20 parts ranging in size up to 30 in. square with draws up to 9 in. deep.

Tongue-and-groove, snap-fit design
Tongue-and-groove, snap-fit design testifies to high-precision forming and CNC trimming and the “memory” of the Kydex acrylic/PVC sheet.

The high-tech unit is complemented by the aesthetics of the newly designed enclosure, which is highly stylized with rounded edges and sleek lines. The original housing was a painted thermoset fiberglass composite. Reasons for switching to pressure forming were better part-to-part consistency and higher output, says Jack Schrieffer, engineering manager for Specialty Manufacturing Inc., a custom thermoformer in San Diego.

According to Schrieffer, the use of air pressure is critical in attaining precision and appearance that rivals injection molding. Vacuum forming of industrial parts is usually done over a male tool, which controls the inside surface of the part and usually has large radii. Pressure forming, however, typically occurs in a female tool, which controls the outside or appearance surface of the part and can achieve tight radii down to 0.005 in. Such tight radii permit more detailed geometries. In addition, in-mold texturing is possible with female tools.

cut-away section
A cut-away section shows the complex geometry for mating parts and also the textured surface and style line that are imparted by the thermoforming mold.

This thermoforming project was a little more complex than usual. The enclosure panels were redesigned with precise tongue-and-groove, snap-fit connections to simplify assembly. The snap-fits are so effective that only 16 fasteners are used to secure the enclosure. The tabs and receiving slots of the connections are formed into the panels, maintaining tolerances within 0.015 in. (0.51 mm).

Schrieffer says pressure forming readily allows the use of undercuts, which are critical to the tongue-and-groove design. Injection molding tools require costly collapsible cores to achieve the same result.

For Specialty Manufacturing, lead times can be as short as four to six weeks and tooling costs for some large parts can be as much as 75% less than for injection molds.

style line receiving groove
Undercut on the edge of one part (right) creates a receiving groove for a snap-fit with the mating component. Another undercut section on the left-hand part creates a tongue for assembly without fasteners. The design results in a style line (left) at the mating seam.

Sheet ‘memory’ is critical
Integrity of the tongue-and-groove connections also relies on the “memory” of the thermoplastic sheet to maintain the shape of the part after the tabs and slots engage. The parts are made of Kydex T, a high-impact, fire-rated acrylic/PVC sheet from Kleerdex Co. “A key to the design is the natural memory of the thermoplastic sheet in achieving a snap-fit,” explains Schrieffer. The material provides a good balance of stiffness and elasticity. Notched Izod impact resistance of 15 ft-lb/in. is significantly better than many competing materials for protection against contact with wheelchairs and gurneys. The material also carries a UL 94V-0/5V fire rating. Sheet thicknesses range from 0.187 to 0.250 in. (4.8 to 6.4 mm).

Because the medical diagnostic unit is produced in limited quantities, typically in the hundreds per year, color consistency is also a special concern. Philips Medical must be able to mix and match components as necessary whether for new units or as replacement parts, with no variation in color. “The material is color-matched to offer the repeatability that is associated with a precision color house,” says Schrieffer.

rear bonnet of the medical device
Specialty Manufacturing v.p. Haydn Forward (front) and engineering manager Jack Shrieffer (rear) hold the rear bonnet of the medical device next to the Maac four-station rotary machine on which it is pressure formed.

Specialty Manufacturing uses a custom four-station rotary pressure former from Maac Corp. The processor opted for a counterpressure floating platen instead of a typical mechanical-lock type. The platen maintains constant pressure, resulting in consistent forming shot-to shot and run-to run, says Schrieffer. Forming-air pressure is applied at 80 psi over the entire platen surface up to 5 x 8 ft. The platen has a deflection of no more than 0.005 in.

Specialty Manufacturing has 50 employees and nine forming machines. The company also does twin-sheet forming and thin-gauge medical packaging.

Tooling and trimming
The tooling, manufactured in-house by Specialty Manufacturing, consists of temperature-controlled, machined aluminum. Schrieffer notes that part appearance hinges on the ability of the sheet to accurately reproduce the acid-etched texture of the aluminum molds. The sheet reproduces mold finish accurately, with no part-to part variation, even among deep-drawn parts. Mold texturing was done by Pacific Texture in Riverside, Calif.

Another essential element of producing tight-tolerance formed parts with high aesthetic requirements today is use of multi-axis CNC trimming equipment. Schieffer notes that a design change can often be accomplished by a simple programming revision such as adjusting the height of a cut or dimension of an opening. “This makes pressure forming even more attractive than injection molding from an overall cost and time-to-market viewpoint,” he says.