EXTRUSION: Are Grooved-Feed Extruders Right for You?
In specific circumstances, this design can increase output and reduce melt temperature. But grooved feed throats are not for every application.
There are basically two types of single-screw extruders, distinguishable primarily by their feed-throat design. Most single-screw extruders have smooth-bore feed throats—basically a smooth pipe surrounding the rotating screw.
Extruders with smooth-bore feed throats are affected a number of ways by the resistance or “head” pressure against which the screw is rotating. As the head pressure increases, a reverse flow (or pressure flow) develops in the screw channels that subtracts from the output (or drag flow) while increasing the melt temperature (because the material is essentially being recirculated back into the screw). This can cause significant problems in extrusion processes that have inherently high head-pressure characteristics resulting from a narrow die gap, such as in blown film, extrusion coating, and thin-wall tubing.
With a smooth-bore feed throat, solids transport of material with the rotating screw is highly dependent on the friction of the polymer particles against the barrel wall. Depending on the polymer and the temperatures, the feed efficiency is typically 15% to 30% based on the channel volume because of “slip” of the polymer particles on the feed-throat wall.
The second type of feed throat has grooves or interruptions machined into the feed-throat wall. Extruders with grooved feed throats resist rotation of the solid polymer particles against the feed-throat wall. This can increase conveying efficiency multiple times. Additionally, because the polymer is much more rapidly compacted into a solid and cannot slip on the feed-throat wall, the screw flights act as a spiral wedge multiplying the pressure development.
As this spiral block of polymer moves down the feed throat, it becomes highly pressurized compared with what occurs in a smooth-bore extruder. In the absence of any melting, which reduces the pressure development, the pressure tends to rise exponentially with groove length. Groove lengths are usually 4D or less because of the exponential rise in pressure and the difficulty in preventing melting from occurring over longer lengths.
Pressures exceeding 12,000 psi have been achieved at the end of the grooved section, so care must be exercised in design to prevent over-pressurization of the barrel. That can be done modifying the design of the grooves themselves, or by designing a decompression section in the screw. This pressure offsets, and in many cases can exceed, the pressure at the discharge. The grooved feed throat is intensively cooled so the material won’t prematurely melt and hinder pressure development.
Since the barrel is essentially a pipe, the pressure from the grooved feed throat transfers through the barrel, counteracting the discharge-pressure resistance. If the feed-throat pressure development exceeds the discharge pressure, the output will exceed the drag flow, resulting in further throughput gains.
To illustrate, I recently observed a test on a 90-mm extruder processing fractional-melt HDPE at a plant I visited. Using a barrier screw design, the output of the grooved-feed-throat extruder was 563 lb/hr, with a melt temperature of 418 F at a screw speed of 95 rpm. Head pressure was 6200 psi. With an essentially identical 3.5-in. smooth-feed-throat extruder having a similarly designed screw, the output was 445 lb/hr at the same screw speed and a slightly lower head pressure. The melt temperature was 432 F. That’s an 26.5% increase in output and a 27° F drop in melt temperature.
That said, before deciding to move to a grooved feed throat, weigh the advantages against the disadvantages for your process.
The advantages of grooved feed throats:
• Reduction or elimination of the effect of high head pressure, resulting in higher output.
• Reduction in melt temperature at same output.
• Stabilized output.
• Not very sensitive to barrel temperatures.
The disadvantages of grooved-feed throats:
• Proportionally more drive power required.
• Performance very sensitive to particle characteristics.
• Generally not suitable for most regrind due to plugging of the grooves.
• Does not work on “soft” polymers like many TPEs due to plugging of the grooves.
• Not as good for compounding additives without extensive mixing sections due to higher specific output.
• Not generally suitable for powdered polymers or additives.
• Can have accelerated screw/barrel wear without accurate balanced design due to higher pressures in feed section.
• Can be unstable with “hard” polymers such as polycarbonate.
• Requires higher volume of cold water for cooling.
• Requires a special screw design, unlike those used for smooth bore extruders.
Grooved-feed technology was developed in Germany in the early 1960s and has been more widely used in Europe than in other parts of the world. However, this design is the standard everywhere for much of HDPE pipe and HMW-HDPE blown film production.
In the late 1960s, Dr. Georg Menges and a group of associates at the IKV at Aachen University published guidelines on using grooved feed throats. While they mostly still apply, new designs have emerged, particularly at the point where the polymer enters the screw, along with varying the shapes of the grooves to accommodate a broader range of polymer particles. Now, grooved-feed designs are more commonplace. Many barrier blown film lines, for example, are equipped entirely with grooved-feed extruders.
Meantime, there also have been many developments in feed-throat “surface improvements.” Though not to be confused with traditional grooved feed throats, these surfaces aim to improve friction at the feed-throat wall by using shallow grooves of various designs. They’ve been shown to significantly improve output with polymers having low feed efficiency, and are effective when processing regrind and fillers. However, where screw design is concerned, they follow the principles of smooth-bore feed throats.
Bottom line: Grooved feed throats have their pros and cons. As a processor, weigh the promise of improved output and lower melt temperature against the disadvantages. Consider them only for situations where they are beneficial overall to the process. Don’t think of them as general-purpose extruders.
Related Content
How Polymer Melts in Single-Screw Extruders
Understanding how polymer melts in a single-screw extruder could help you optimize your screw design to eliminate defect-causing solid polymer fragments.
Read MoreHow Much L/D Do You Really Need?
Just like selecting the extruder size and drive combination, the L/D should be carefully evaluated.
Read MoreFully Automated Extrusion Process Enables Use of Composites for Manufacturing Pressure Tanks
Amtrol was looking for a more cost-effective means to produce thin-wall liners for a new line of pressure tanks. With the help of a team of suppliers, they built one of the world’s most sophisticated extrusion lines.
Read MoreWhy Compression Ratio is Important
Compression ratios have been pretty much standardized over the years, based on what has typically worked before. But there are quite a few variables that must be considered in order to get the optimum performance from your screw.
Read MoreRead Next
People 4.0 – How to Get Buy-In from Your Staff for Industry 4.0 Systems
Implementing a production monitoring system as the foundation of a ‘smart factory’ is about integrating people with new technology as much as it is about integrating machines and computers. Here are tips from a company that has gone through the process.
Read MoreTroubleshooting Screw and Barrel Wear in Extrusion
Extruder screws and barrels will wear over time. If you are seeing a reduction in specific rate and higher discharge temperatures, wear is the likely culprit.
Read MoreProcessor Turns to AI to Help Keep Machines Humming
At captive processor McConkey, a new generation of artificial intelligence models, highlighted by ChatGPT, is helping it wade through the shortage of skilled labor and keep its production lines churning out good parts.
Read More